1 Introduction of Solid Carbide Tools
Solid carbide tools are increasingly widely used in the aerospace industry, mould manufacturing industry, automobile manufacturing industry, machine tool manufacturing industry and other fields, especially in the field of high-speed cutting. In the field of high-speed cutting, due to the high standards for tool safety, reliability and durability, the internal and surface quality requirements of integral carbide tools are also more stringent. With the continuous improvement of the internal quality of carbide rods, especially ultra-fine carbide materials, the surface quality of integral carbide tools has received more and more attention.

As we all know, the service life of carbide tools is not only related to their wear resistance but also often manifests in abnormal failures such as chipping, broken edges and fractures. Surface defects such as grinding cracks of tools after grinding are one of the important reasons for such abnormal failures. These surface defects include powder metallurgy manufacturing defects (such as delamination, cracks, poor pressing, holes, etc.) of carbide rods exposed to the surface after grinding, and grinding cracks caused by unreasonable grinding on the grinding surface during the grinding process. Grinding cracks are more common. The grinding crack defects of solid carbide tool products are very harmful. It is of great practical significance to analyze and discuss the causes of grinding cracks in solid carbide tools and propose process improvement measures to effectively prevent grinding cracks.
2 Analysis of the causes of grinding cracks in solid carbide tools
2.1 Grinding characteristics of solid carbide tools
Due to high hardness, high brittleness and low thermal conductivity, cemented carbide materials bring great difficulties to the sharpening of tools, especially solid carbide tools with large grinding allowances. High hardness requires greater grinding pressure, low thermal conductivity does not allow excessive grinding heat, and high brittleness leads to a high tendency to produce grinding cracks. Therefore, for the sharpening of cemented carbide tools, it is required that the grinding wheel has good self-sharpening properties, reasonable sharpening technology, and good cooling to provide better heat dissipation conditions and reduce the occurrence of grinding cracks.
Generally, when sharpening carbide tools, the temperature is higher than 600℃, and the surface layer of the tool will produce oxidation discolouration, causing grinding burns of varying degrees. In severe cases, it is easy to cause cracks in the carbide tool. These cracks are generally very small, and the grinding surface near the cracks often has the colours of tungsten oxides with different oxygen indices, such as blue, purple, brown, and yellow. After breaking along the cracks, the fracture source of the crack fracture often has traces of severe burns. The entire crack section is often clearly demarcated from the fresh section due to the infiltration of grinding oil.
Traditional silicon carbide grinding wheels for grinding carbide have been gradually phased out due to their low grinding efficiency, large grinding force, poor self-sharpening, and high local temperature of the grinding contact area (up to about 1100°C), which result in poor tool edge quality, poor surface roughness, and high scrap rate. Diamond grinding wheels, on the other hand, are widely used in the grinding of carbide tools due to their high grinding efficiency, small grinding force, good self-sharpening, sharp diamond edges, not easy to passivate, and low local temperature of the grinding contact area (generally around 400°C). However, in the grinding process of solid carbide tools with diamond grinding wheels, due to the large grinding allowance, improper selection of processing methods, diamond tool characteristics, and grinding systems, the local instantaneous temperature of the tool grinding contact area surface will be high, resulting in grinding cracks.
2.2 Analysis of the generation mechanism of grinding cracks in solid carbide tools
The diamond grinding process used in the manufacture of carbide tools can deteriorate or improve the physical mechanical properties of the tool surface layer. The basic parameters that determine the quality of the surface layer are micromorphology (i.e. surface roughness), structure and substructure of the surface layer, and the value and distribution of the first type of residual stress.
After sintering, cemented carbide usually has a surface roughness of not less than Rz5µm. Diamond processing can ensure that Rz is not less than 2µm. The depth of micro-roughness in the range of Rz = 1 to 5µm does not actually affect the life index of cemented carbide. During the grinding process, the fine crystal structure parameters inside the cemented carbide grains also change, and the embedded crystal blocks are broken (coherent dispersion area), and its value is reduced by an order of magnitude, from (10 to 15) × 10-5mm to (10 to 15) × 10-6mm. The grain micro-distortion value (Δd/d, second type of stress) changes and the surface layer performance also changes accordingly. However, in fact, no direct relationship has been found between the change of fine crystal structure parameters and the life of cemented carbide. Therefore, under cyclic loads (such as milling force), the service life of cemented carbide has no direct correlation with the structure and substructure of the surface layer and is not primarily determined by the surface roughness, but by the residual stress state of the surface layer, that is, the value of the type I residual stress and its distribution along the cross-section play a decisive role in the strength and life of cemented carbide.
The formation of residual compressive stress in the surface layer prompts the fracture source to migrate to a layer deeper from the surface with less load, inhibiting the initiation and expansion of cracks, which increases the strength and life; at the same time, as the distribution depth of the residual compressive stress layer in the surface layer of cemented carbide increases, its strength and life gradually increase. The residual tensile stress formed in the surface layer promotes the initiation and expansion of cracks, which is a necessary condition for the generation of cracks and reduces the strength and life.
However, the surface after grinding often has both residual compressive stress and tensile stress. Therefore, the ideal state of the grinding surface layer should be that the higher the residual compressive stress value of the surface layer, the better, and the deeper the residual compressive stress layer distribution, the better; the lower the residual tensile stress value of the near-surface layer, the better, the thinner the residual tensile stress layer, the better, and the deeper the maximum tensile stress value is from the surface, the better. On the contrary, the shallow compressive stress distribution of the surface layer and the excessively high tensile stress value of the near-surface layer are the main reasons for the initiation of grinding cracks. Therefore, the generation of residual tensile stress should be minimized and avoided during the grinding process.
In most cases, residual tensile stress (originating from heat) is generated in the surface layer of cemented carbide products after sintering, and this tensile stress value can reach 500-1000MPa. The depth of this stress layer is not more than 5-7µm, and the stress penetration depth does not exceed 30-40µm. The closer to the surface, the higher its value; the higher the cobalt content, the higher its value. Therefore, the bending strength value (TRS value) and fatigue life value of cemented carbide after sintering are very low. However, the grinding allowance is often greater than 0.1mm, so the subsequent grinding process can completely eliminate the residual tensile stress in the sintered alloy after removing the surface layer of the cemented carbide, and form a new stress state. It can be seen that the residual stress caused by the sintering process has no effect on the formation of residual stress during the grinding process.
During the grinding process, there are two main factors that affect the surface state of the tool: the applied force and the local temperature.
The effect of the applied force on the alloy surface will cause irreversible plastic deformation, structural changes and phase changes accompanied by an increase in unit volume, thereby leading to the formation of residual compressive stress, improving bending strength, fatigue strength, impact toughness, hardness, wear resistance and service life, that is, a strengthening process occurs;
The effect of local temperature on the alloy surface will produce uneven thermoplastic deformation, and structural and phase changes in the surface layer accompanied by a decrease in unit volume, thereby leading to the formation of residual tensile stress, reducing bending strength, fatigue strength, impact toughness, hardness, wear resistance and service life, that is, a weakening process occurs.
Therefore, whether the final surface state of the carbide tool is strengthened or weakened, whether the residual compressive stress is dominant or the residual tensile stress is dominant, depends on whether the action on its surface during the grinding process is mainly force or temperature. When the local instantaneous temperature of the grinding contact zone reaches a certain level (sometimes up to 1000°C or above) during the grinding process, it will form a shallow compressive stress distribution on the surface layer and an excessively high tensile stress value near the surface layer. The residual tensile stress promotes the initiation and expansion of cracks, and its value is so large that it may even exceed the breaking strength of the material and form tiny cracks. Sometimes no cracks are generated after grinding, but during grinding or use, when the surface layer is removed, the residual stress of the lower layer loses balance and cracks appear. During diamond processing, the local instantaneous temperature of the grinding contact zone on the tool surface will depend on the processing method, diamond tool characteristics and grinding system.
3. Improvement of the Grinding Process of Solid Carbide Tools
3.1 Grinding Process Factors Affecting Grinding Cracks
As mentioned above, the grinding cracks on the surface of solid carbide tools are mainly caused by the excessively high local instantaneous temperature of the grinding contact zone during the grinding process, which forms a shallow compressive stress distribution on the grinding surface layer and an excessively high tensile stress value near the surface layer that exceeds the breaking strength of the material. Therefore, the generation of instantaneous high temperatures should be minimized and avoided during the grinding process, thereby reducing and avoiding the generation of residual tensile stress.
The instantaneous high temperature during the grinding process often causes changes in the mechanical properties of the grinding surface layer. This instantaneous high temperature can reach more than 1000°C, causing grinding burns on the surface layer of the tool. Grinding burns will destroy the surface layer of the tool, deteriorate the quality of the workpiece surface, and seriously affect the strength, wear resistance and service life of the tool; in severe cases, cracks will also occur. Therefore, it is necessary not only to prevent the generation of grinding cracks but also to avoid grinding burns. During diamond processing, the local instantaneous temperature of the tool surface will depend on the processing method, diamond tool characteristics and grinding system.
The practice has proved that the greater the linear speed and radial feed of the diamond grinding wheel, the higher the hardness of the grinding wheel, the finer the grinding wheel grain, the lower the thermal conductivity of the tool material and the more severe the grinding wheel wear, the greater the grinding temperature, and the easier it is to produce grinding cracks and grinding burns.
To control and avoid grinding cracks and grinding burns, two measures must be taken: one is to reduce the generation of grinding heat, and the other is to accelerate the transmission of grinding heat.
The way to reduce grinding heat is:
Appropriately reduce the linear speed of the diamond grinding wheel, reduce the radial feed (rough grinding-fine grinding-polishing in separate steps), select a softer diamond grinding wheel, reduce the contact area between the workpiece and the grinding wheel, reasonably select the grinding wheel grain size according to the grinding requirements, always keep the grinding wheel under sharp conditions, and select appropriate grinding coolant to reduce the friction between the abrasive and the workpiece.
The measures to accelerate the heat transfer of grinding are
In addition to appropriately increasing the workpiece speed and axial feed rate, the main method is to adopt effective cooling methods; in order to improve the cooling effect, spray cooling, high-pressure cooling, internal cooling and cooling oil with low kinematic viscosity can be used. In addition, during fine grinding, reducing the feed rate and appropriate light grinding can effectively reduce the residual stress in the surface layer.
In summary, in order to improve productivity and grinding efficiency, while obtaining a better grinding surface quality, our method is to use a lower grinding wheel linear speed and a larger radial feed rate at the beginning, reduce the feed rate and increase the grinding wheel linear speed for the last few times, and perform light grinding, which can improve the grinding surface quality. In order to further improve the grinding surface quality, spray cooling and high-pressure cooling can also be used, and appropriate cutting fluids can be selected. At the same time, the grinding wheel can be reasonably selected and the grinding wheel can be finely dressed according to the processing object.
The principle of selecting grinding parameters is: grinding parameters are to select lower grinding wheel linear speed, larger radial feed rate, axial feed rate and workpiece speed as much as possible under the conditions of ensuring low grinding temperature and high grinding surface roughness. Since the linear speed and radial feed of the grinding wheel have the greatest impact on the quality of the grinding surface layer, the steps for selecting grinding parameters are: first select a larger workpiece speed, then select the axial feed, and finally select the linear speed and radial feed of the grinding wheel.
3.2 Grinding process improvement measures to prevent grinding cracks
1) Select the appropriate coolant and cooling method
2) Replace domestic cooling oil with imported cooling oil with lower kinematic viscosity, and improve the cooling method so that the cooling oil is always cooled in the grinding contact area, and the oil temperature is controlled below 2315℃ (air conditioning control), and at the same time increase the oil pump pressure of the tool grinder to enhance the cooling effect during grinding.
3) Choose the right diamond grinding wheel.
Metal bond diamond grinding wheels are mainly used for rough and fine grinding of the rough grooving process (groove grinding) due to their good thermal conductivity, high grinding force and high grinding efficiency. High-temperature resin-bond diamond grinding wheels can also be used for this process, but the wear is relatively large; resin-bond diamond grinding wheels have good lubricity, small grinding force and good self-sharpening properties. Medium and medium soft resin bond diamond grinding wheels or diligent grinding wheels are selected to keep the grinding wheels sharp at all times. They are mainly used for rough and fine grinding of the tooth opening process (the general term for the front and rear blades, end tooth grooves, and offset back removal processes).
The concentration of diamond grinding wheels should be 75% to 100%, the grit of metal bond grinding wheels should be 120 to 140 mesh, and the grit of resin bond grinding wheels (RVD) should be 80 to 120 mesh for rough grinding and 200 to 240 mesh for fine grinding. If all imported grinding wheels with good quality are used, the grinding efficiency and surface roughness of the tool will be higher than those of domestic grinding wheels.
4) Choose reasonable grinding parameters
Take the grinding of solid carbide two-edge spiral end mills on the UWIE212 CNC tool grinder (15kW) of SAACKE, Germany as an example. For the rough grooving process (groove grinding), the diamond grinding wheel linear speed is 14-20m/s, the machine tool axial feed speed is 50-200mm/min, the machine tool radial feed is 210-510mm for rough grinding, and 0.2-0.5mm for fine grinding; for the toothing process (the front and rear blades, end tooth grooves, and offset back removal processes), the diamond grinding wheel linear speed is 14-24m/s, the machine tool axial feed speed is 100-400m/min, the machine tool radial feed is 0.3-1.0mm for rough grinding, and 0.05-0.1mm for fine grinding. When grinding the front and rear blades, non-feed return polishing is also used to improve the surface roughness. If imported grinding wheels are used, it is allowed to select a higher grinding wheel linear speed and larger radial feed rate than domestic grinding wheels.
3.3 Verification of the effect of grinding process improvement measures
After the grinding process was improved, more than 6,800 solid carbide tools (of which nearly 4,000 were high-speed milling cutters) were inspected using the same post-emulsification fluorescent penetrant detection method. The results show that: not only the grinding surface quality of the tool is greatly improved, but the grinding crack rate is gradually reduced from nearly 20% before the process improvement to 15%, 10%, 6% after the process improvement, and finally to below 0.5% of the best-improved process. The grinding burn of the tool surface (bright, white instead of blue, purple, brown, yellow, black, dark) and the surface roughness (Rz0.2~0.8µm) are also significantly improved;
Moreover, the grinding efficiency is also improved. Taking a 20mm diameter two-edged solid carbide high-speed milling cutter as an example, it takes 30~40min to complete the grinding of each tool before the process improvement, but only 20~30min after the process improvement. If imported cooling oil and imported diamond grinding wheels with better quality are used, the grinding efficiency corresponding to the best-improved process can be increased to 14~20min per piece.
4. Conclusion
The main reason for grinding cracks in solid carbide tools is that the inappropriate grinding process and parameters lead to excessive local instantaneous temperature in the grinding contact area, causing excessive tensile stress values in the near-surface layer exceeding the breaking strength of the material.
The highly sensitive hydrophilic post-emulsification fluorescent penetrant flaw detection method can effectively detect surface defects such as grinding cracks in solid carbide tools; this method is recommended to be widely used in the field of quality assurance technology for solid carbide tools.
The generation of grinding cracks and grinding burns can be effectively prevented by improving and optimizing the grinding process and grinding parameters of solid carbide tools