1. Wear of carbide hob cutter teeth
1) Normal wear forms of teeth
When carbide hob cutters are used normally, the teeth will show several normal wear forms, including slight wear, moderate wear, and severe wear. Due to the high hardness and low bending strength of carbide, it is sensitive to the impact of intermittent cutting.
Sometimes, some tiny brittle chipping will occur during use. This tiny chipping is a common initial wear form when high-hardness tools are intermittently cut. Generally, it does not affect continued use so it can be regarded as a form of normal wear.
2) Abnormal wear forms of carbide hob cutter teeth
When carbide hobs cut teeth, due to the influence of alternating cutting force and cutting heat, the teeth are repeatedly subjected to mechanical shock and rapid temperature changes. In addition, the physical and mechanical properties of carbide blades, grinding thermal stress, etc., as well as improper hob re-grinding and improper impact when the tool is not aligned, will cause some abnormal damage to the teeth, including cracks, chipping, peeling, etc.

2. Analysis of abnormal wear of carbide hob cutter teeth
The main reasons for abnormal damage to carbide hob teeth during use are:
(1) Failure to comply with grinding specifications during hob regrinding can easily cause abnormal damage to hob teeth.
After the carbide hob teeth wear reaches the blunt standard, it needs to be regrinded. If the diamond grinding wheel is improperly selected and the blade is not properly sharpened during regrinding, a large amount of grinding heat will be generated during the grinding of the tool, inducing cracks in the carbide, which will continue to expand during the cutting process and quickly develop into chipping or peeling damage.
(2) Failure to comply with hob-cutting specifications during use can cause abnormal damage to the teeth.
During the cutting process, if the carbide cutting load is too large, the speed is too high, the workpiece is too hard, etc., the carbide teeth will be cracked and multi-ring fatigue damage will occur due to mechanical impact and thermal fatigue.
In addition, due to the chips squeezing into the cutting area, hard spots and impurities on the tooth surface and some other accidental reasons, it will also cause chipping or cutting (large chipping).
Various abnormal damage to carbide teeth will seriously affect the service life of carbide hob cutters, so they should be avoided as much as possible.
3. Some suggestions on the processing and use of carbide hob cutters
1) Correctly regrind the hob.
(1) Correctly select diamond grinding wheels.
According to the processing requirements, processing methods and processing conditions, it is recommended to use resin-bonded diamond disc-shaped or bevel-shaped grinding wheels with a diamond concentration between 75~100% and a particle size between 150~180#. The softness and hardness of the grinding wheel bond and the self-sharpening of the grinding wheel must be appropriate.
(2) Correctly select the grinding specifications.
According to the processing requirements, processing methods and processing conditions, it is recommended that the grinding wheel linear speed be 15~20ms (dry grinding) and 20~30ms (wet grinding); the grinding depth is 0.01~0.02mm.
(3) It is advisable to choose wet grinding and select the cutting fluid correctly.
When grinding carbide tools with diamond grinding wheels, a large amount of grinding heat will be generated.
Excessive heat will damage the resin of the grinding wheel, clog the working surface, and induce cracks in the carbide. In order to improve the grinding performance of the diamond grinding wheel, reduce grinding wheel consumption, and improve processing quality, cutting fluid should be used during grinding.
Based cutting fluid has little effect on the maintenance of machine tools, but has poor cooling performance. It is best to use specially formulated water-based cutting fluid. The cutting fluid flow rate is generally 3~8L/min.
(4) Timely dressing of diamond grinding wheels.
After a period of use, the working surface of the diamond grinding wheel will become clogged and the shape will change. In order to restore the grinding ability and shape accuracy of the grinding wheel, the diamond grinding wheel should be dressed as necessary.
It is recommended to use silicon carbide oilstone for dressing. At the working speed of the diamond grinding wheel, the silicon carbide oilstone is moved relatively along the working surface of the grinding wheel, which can effectively clear the blockage of the grinding wheel working surface and have a certain shape dressing effect. According to the working conditions when dressing the grinding wheel, the silicon carbide oilstone can be held by hand or clamped with flat-nose pliers.
(5) Issues that need attention during grinding.
The moving speed of the workbench should be kept between 0.8 and 1.2 m/min. During the grinding process, after 4 to 5 times of feed grinding, the workbench should choose 1 to 2 times of non-feed grinding. The purpose is to adjust and control the grinding amount to avoid excessive grinding amount, resulting in excessive grinding heat, which is most likely to cause tooth cracking and obvious cracks. After grinding to size, the workbench does not feed and then performs 5 to 8 back-and-forth strokes of non-feed grinding.
2) Strictly comply with the hob cutting specifications.
(1) Correctly select the hob cutting speed.
If the cutting speed is too high during the hobbing of the hard gear surface, fatigue damage to carbide cutter teeth will occur. If the speed is too low, carbide cutter teeth will produce low-speed chipping and deteriorate the surface quality.
The linear speed is usually 30~80m/min. Considering the hardness of the workpiece, machine tool conditions and tool performance, it is recommended that the linear speed be selected as 30~55m/min.
(2) Correctly select the hob feed rate.
The feed rate during the hobbing of the hard gear surface should be determined according to the machine tool performance and processing requirements. The larger the feed rate, the higher the hobbing efficiency, while the wear of the cutter teeth is reduced. For semi-finishing hobbing before grinding, if the machine tool performance allows, a larger feed rate should be used as much as possible to achieve a better tooth-cutting effect. However, the axial feed mark of the hob will cause tooth surface waviness and convert into tooth shape error to a certain extent, and its value is proportional to the square of the axial feed rate.
From the perspective of gear-cutting accuracy, the axial feed rate during the fine rolling of the hard gear surface should not be too large or too small. Generally, f=1~3.0mm/r can be used.
(3) Correctly select the cutting thickness.
The influence of cutting thickness on the hobbing accuracy of hard gear surface is mainly due to the change of cutting force caused by uneven cutting thickness and the excessive wear of cutter teeth caused by excessive cutting thickness. Uneven cutting volume causes changes in cutting force and causes different cutter clearance, resulting in a certain tooth profile error. When the cutting thickness exceeds 0.2mm, the wear of the cutter teeth accelerates and the tooth profile error of the cut gear will also increase. Therefore, for the fine rolling of the hard gear surface, it is best to cut off the processing allowance twice (or three times) to make the cutting thickness uniform during the last fine rolling and limit the cutting volume to between 0.1~0.2mm to ensure the accuracy of fine rolling.